Examples of Toughening Modification Formula

Publish Time: 2018-12-10     Origin: Site


Examples of toughening modification formula

Raw material

Addition ratio

PP(F401)

13

PP(1340)

20

Acrylic acid grafted polypropylene

25

POE(8180)

12

Antioxygen(1010)

0.1

Antioxygen(DLTP)

0.1

CaCO3(2500mesh)

30

Coupling agent of organic titanate

0.3


Processing technology: 

weight according to formula, 

initial mix with high speed mixer

blend and granulate with twin-screw extruder.



Application: 

coated automobile bumper cover fabric.


 

Raw material

Addition ratio

PP(EPF30R)

100

POE(DOW)

5

BaSO4

30

β nucleating agent

0.3


Application: 

weatherproof rigid toughened PP                              


 


Filler Modification: How To Properly Convey And Feed Powdered Calcium Carbonate in Plastics, And Beware of Particle Interactions

Choosing The Right Carrier for Color Masterbatches in TPE Pelletizing

How To Select Additives for Plastics

Why Recycled Plastic Is More Expensive Than Virgin Plastic? 3 Key Reasons Explained

Why Is Recycled Plastic Praised But Not Popular?